西安雙相不鏽鋼管的焊接要求

日期:2025-12-08 04:50
瀏覽次數:0
摘要:<span style="font-family:宋體;font-size:small;"> </span> <p style="margin:0cm 0cm 0pt;"> <span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;"><span style="font-size:small;">西安雙相不鏽鋼管的焊接要求</span></span> </p> <span style="font-family:宋體;font-size:small;"> </span> <p style="margin:0cm 0cm 0pt;"> <span style="font-size:small;"><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">在石油化工裝置中一種新型鋼材</span><span style="font-family:'Times New Roman';"><span lang="EN-US">-</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">雙相不鏽鋼的應用越來越多。因為雙相不鏽鋼的屈服強度是普通不鏽鋼的</span><span style="font-family:'Times New Roman';"><span lang="EN-US">2</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">倍,抗腐蝕性能(特彆是在腐蝕性介質中)明顯優於普通不鏽鋼,在石油化工裝置施工中多用在很重要的位置。因此,一般雙相不鏽鋼的焊縫要求</span><span style="font-family:'Times New Roman';"><span lang="EN-US">100%RT</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">檢驗,對其焊接接頭的綜合性能的要求也高於一般奧氏體不鏽鋼。所以,必須選派焊接經驗豐富的奧氏體不鏽鋼焊工,經培訓和考試合格後,才能持證上崗進行焊接作業。</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> 1&nbsp; &nbsp; </span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;"><span style="font-size:small;">焊接性分析</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> </span></span><span style="font-size:small;"><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">雙相不鏽鋼焊接時,焊接熱影響區(</span><span style="font-family:'Times New Roman';"><span lang="EN-US">HAZ</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">)</span></span><span style="font-family:'Times New Roman';font-size:small;"> </span><span style="font-size:small;"><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">存在高溫區和低溫區,低溫區基本處於</span><span style="font-family:'Times New Roman';"><span lang="EN-US">δ+γ</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">(鐵素體</span><span style="font-family:'Times New Roman';"><span lang="EN-US">+</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">奧氏體)平衡組織,而高溫區幾乎為單相</span><span style="font-family:'Times New Roman';"><span lang="EN-US">δ</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">組織,因為焊縫根部和表麵</span><span style="font-family:'Times New Roman';"><span lang="EN-US">N</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">的擴散,導致靠近焊縫表麵的部位,由於</span><span style="font-family:'Times New Roman';"><span lang="EN-US">N</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">的損失,鐵素體增加,從而促進氮化物的產生,使焊接接頭性能惡化,焊接采用高線能量時,可以得到較多的</span><span style="font-family:'Times New Roman';"><span lang="EN-US">γ</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">相,鐵素體含量低會促進</span><span style="font-family:'Times New Roman';"><span lang="EN-US">δ</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">相產生,所以容易產生</span><span style="font-family:'Times New Roman';"><span lang="EN-US">δ</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">相和粗晶組織;線能量較低時,得不到足夠的</span><span style="font-family:'Times New Roman';"><span lang="EN-US">γ</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">相。如果焊接金屬中</span><span style="font-family:'Times New Roman';"><span lang="EN-US">δ</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">相過多,</span><span style="font-family:'Times New Roman';"><span lang="EN-US">N</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">很容易與</span><span style="font-family:'Times New Roman';"><span lang="EN-US">cγ</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">形成化合物,而且析出二次</span><span style="font-family:'Times New Roman';"><span lang="EN-US">γ</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">變為針狀和羽毛狀,具有魏氏體組織特性,導致焊接接頭力學性能和耐腐蝕性下降。雙相鋼一般不會產生</span><span style="font-family:'Times New Roman';"><span lang="EN-US">δ</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">相,但如果焊接線能量較高,導致使焊接頭塑性大幅度下降。</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> 2&nbsp; &nbsp; </span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;"><span style="font-size:small;">焊接工藝</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> 2.1&nbsp; &nbsp; </span></span><span style="font-size:small;"><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">工藝參數及電特性(見表</span><span style="font-family:'Times New Roman';"><span lang="EN-US">2</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">)</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> 2.2&nbsp; &nbsp; </span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;"><span style="font-size:small;">焊接方法</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> </span></span><span style="font-size:small;"><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">雙相不鏽鋼薄壁管全部采用</span><span style="font-family:'Times New Roman';"><span lang="EN-US">GTAW</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">焊接,直流正極性。</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> 2.3&nbsp; &nbsp; </span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;"><span style="font-size:small;">焊接設備</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> </span></span><span style="font-size:small;"><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">焊機采用高頻引弧焊機,直流正極性,鎢極直徑</span><span style="font-family:'Times New Roman';"><span lang="EN-US">Φ2.5mm</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">,鎢極端頭用磨光機磨出錐形,采用大噴嘴。</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> 2.4&nbsp; &nbsp; </span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;"><span style="font-size:small;">氣體保護</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> </span></span><span style="font-size:small;"><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">焊接保護氣體采用混合氣體</span><span style="font-family:'Times New Roman';"><span lang="EN-US">Ar97.5%+N2.5% </span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">進行保護,保護氣采用成品混合氣,要求生產的成品混合比為</span><span style="font-family:'Times New Roman';"><span lang="EN-US">Ar97.5%+N2.5%</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">,由於混合氣體中</span><span style="font-family:'Times New Roman';"><span lang="EN-US">Ar</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">比</span><span style="font-family:'Times New Roman';"><span lang="EN-US">N</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">多,放置一段時間後將會產生分層,影響氣體保護效果,現場所采用搖勺或加氣體分配器進行配比,確保氣體保護質量。</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> 2.5&nbsp; &nbsp; </span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;"><span style="font-size:small;">環境要求</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> </span></span><span style="font-size:small;"><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">雙相不鏽鋼焊接要求環境清潔。無鐵離子汙染,預置工作將在室內進行,地麵采用膠皮隔離、安裝必須做好環境保護。采用防風防塵設施,環境溫度</span><span style="font-family:'Times New Roman';"><span lang="EN-US">70</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">℃,相對溫度</span><span style="font-family:'Times New Roman';"><span lang="EN-US">≤90%</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">,所有與雙相鋼焊接坡口相接觸的,如:焊材、工具、手套等,都必須無鐵鏽汙染。坡口均采用坡口機加工,坡口角度為單邊</span><span style="font-family:'Times New Roman';"><span lang="EN-US">30°±2.5°</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">,鈍邊</span><span style="font-family:'Times New Roman';"><span lang="EN-US">0~ 0.5mm</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">,單麵坡口(見附圖),加工坡口不允許母材產生過燒變色;其兩側各</span><span style="font-family:'Times New Roman';"><span lang="EN-US">50mm</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">以內的內外表麵要進行嚴格清理,清理程序是磨光機打磨、丙酮(或無水乙醇)清洗,清洗後不能直接進行焊接作業,待坡口端麵晾乾後方可焊接作業;焊絲也用沾丙酮(或無水乙醇)的海綿擦拭乾淨。對鐵離子、水鏽、油、灰塵、油漆、記號筆印都必須清理乾淨,防止其影響化學成份和機械性能。另外,還要注意坡口形狀必須無凹凸和劃痕,這樣焊接時電弧在焊道的每一點上都能保證停留相同的時間,焊接線能量才能確保一致。</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> 2.6&nbsp; &nbsp; </span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;"><span style="font-size:small;">焊接措施</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> </span></span><span style="font-size:small;"><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">儘量采用多層焊,因為後續焊道對前層焊道有熱處理作用,焊縫中的</span><span style="font-family:'Times New Roman';"><span lang="EN-US">δ</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">相進一步轉化為</span><span style="font-family:'Times New Roman';"><span lang="EN-US">γ</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">相,使焊接接頭的組織和性能顯著改善,而後一道焊縫處於非工作介質麵,因為對焊接接頭影響不大,保護氣采用</span><span style="font-family:'Times New Roman';"><span lang="EN-US">Ar97.5%+N2.5%</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">。因為焊接根部保護氣體中加氮氣增加焊縫金屬氮量,由於采用多層焊工藝,焊接材料中含</span><span style="font-family:'Times New Roman';"><span lang="EN-US">N</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">量與母材相當,而後一道焊縫處於非工作介質麵,因為對焊接接頭影響不大,采用合適的線能量焊接,使焊接接頭得到足夠的</span><span style="font-family:'Times New Roman';"><span lang="EN-US">γ</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">相,使</span><span style="font-family:'Times New Roman';"><span lang="EN-US">Cγ</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">、</span><span style="font-family:'Times New Roman';"><span lang="EN-US">N1 </span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">和</span><span style="font-family:'Times New Roman';"><span lang="EN-US">M</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">有足夠的時間擴散。</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> 2.7&nbsp; &nbsp; </span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;"><span style="font-size:small;">坡口的組對及點焊</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> </span></span><span style="font-size:small;"><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">坡口組對前應仔細檢查坡口管徑是否相同,錯邊應控製在</span><span style="font-family:'Times New Roman';"><span lang="EN-US">0.5~1mm</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">之間,並用磨光機打磨清理坡口及坡口正反麵兩側</span><span style="font-family:'Times New Roman';"><span lang="EN-US">50mm</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">以內的表麵,並用丙酮擦試乾淨,坡口打磨時不允許使母材產生過熱變色。點焊時,應采用與正式的焊接工藝相同的參數,點焊長度為</span><span style="font-family:'Times New Roman';"><span lang="EN-US">7~8mm</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">,高度為</span><span style="font-family:'Times New Roman';"><span lang="EN-US">2~ 3mm</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">,點焊點應為過橋型式,不應焊透,以防內部氧化,點焊電流不宜過大,點焊點位置應在組對管子的上部及兩側,點固三點,從第四點起焊,當焊到點焊時,將點固點打磨清理乾淨,焊縫組對間隙應控製在</span><span style="font-family:'Times New Roman';"><span lang="EN-US">2~2.5mm</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">,間隙不應過大,並留有</span><span style="font-family:'Times New Roman';"><span lang="EN-US">0~0.5mm</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">的鈍邊。</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> 2.8&nbsp; &nbsp; </span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;"><span style="font-size:small;">雙相不鏽鋼的焊接操作</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> </span></span><span style="font-size:small;"><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">雙相不鏽鋼焊接時,應采用正反麵氣體保護焊,正麵背麵都應采用混合氣體</span><span style="font-family:'Times New Roman';"><span lang="EN-US">Ar97.5%+N2.5% </span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">進行保護,焊接前不得在焊件表麵引弧和試驗電流,焊接時應按指定的焊接作業指導書進行施焊。在焊接前,管子兩端用布或膠皮封好,並留有進氣孔和排氣孔,焊縫間隙用膠布貼好,並留有</span><span style="font-family:'Times New Roman';"><span lang="EN-US">20~30mm</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">的長度,使管子內部的空氣能夠排出,確保焊縫內部的氣體保護效果。焊接時,焊槍不宜擺動,手法要穩,嚴格控製線能量,儘量采用小焊絲,嚴格控製電流,弧長儘量壓低控製電壓,儘量用大噴嘴,提高氣體保護效果,降底</span><span style="font-family:'Times New Roman';"><span lang="EN-US">O</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">、</span><span style="font-family:'Times New Roman';"><span lang="EN-US">H</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">汙染;引、收弧避開點焊點,防止產生二次</span><span style="font-family:'Times New Roman';"><span lang="EN-US">γ</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">和</span><span style="font-family:'Times New Roman';"><span lang="EN-US">δ</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">相,引弧點必須在焊道內進行,不能在母材表麵引弧,防止</span><span style="font-family:'Times New Roman';"><span lang="EN-US">F</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">量超標;點焊點打磨後,封底焊焊接過程中通過觀察焊道顏色來確定焊接氣體保護效果,采用混合氣體施焊時焊道好為金黃色,稍差一些為黃銅色,儘量減少焊縫發藍,杜絕焊道發灰和發黑,並嚴格控製層間溫度,控製熔池在紅熱狀態下停留時間。一般來講,隻要保證在</span><span style="font-family:'Times New Roman';"><span lang="EN-US">5~15s</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">時間內熔池由紅轉至常規顏色,就能達到要求。打底焊的層間溫度</span><span style="font-family:'Times New Roman';"><span lang="EN-US">≤100</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">℃,可用遠紅外激光測溫儀測量。當層間溫度<</span><span style="font-family:'Times New Roman';"><span lang="EN-US">100</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">℃時,才能進行下一層焊接,焊接電流不能超過打底焊的電流,焊**層必須認真清理前一層焊道,除消除雜質外,連氧化色也需磨去,焊縫內部餘高應控製在</span><span style="font-family:'Times New Roman';"><span lang="EN-US">0.5 ~1mm</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">;焊縫收弧時應將弧坑填滿,多層焊的層間接頭應相互錯開,如果焊接作業時不慎出現夾鎢時,應停止焊接作業,用磨光機消除鎢點,鎢極端部重新磨尖,達到要求後方可重新進行焊接作業,要求與開始焊接作業相同。</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> 2.9&nbsp; &nbsp; </span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;"><span style="font-size:small;">焊後清理和焊接檢驗</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> </span></span><span style="font-size:small;"><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">雙相不鏽鋼的焊後清理也很重要,氧化色必須**,因為氧化色下麵就是貧鉻層,若不去除將會導致耐蝕性能下降,去除氧化色可用專用不鏽鋼絲刷趁熱擦刷;也可用酸或酸洗膏清洗。去除焊接飛濺,打磨收起弧點,去除咬邊和粗毛刺??捎幂^細的砂輪片或拋光砂輪片研磨,杜絕粗糙打磨痕跡,否則易造成縫隙腐蝕;油汙、著色劑、色筆印、灰塵均有可能成為孔腐蝕和縫隙腐蝕的起始點,可用硝酸</span><span style="font-family:'Times New Roman';"><span lang="EN-US">+</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">氫氟酸清洗,然後清水衝洗乾淨;焊工應對焊道表麵進行清理,要求外觀良好,寬度以每邊蓋過坡口邊緣</span><span style="font-family:'Times New Roman';"><span lang="EN-US">2mm</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">為宜,角焊縫的焊腳高度符合設計規定外形平穩過渡,焊縫不允許咬邊、裂紋、未焊透、氣孔、夾雜存在。射線探傷方法按《壓力容器無損檢測》</span><span style="font-family:'Times New Roman';"><span lang="EN-US">JB4730-g4</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">執行,所有焊道必須進行硬度測定,測定母材</span><span style="font-family:'Times New Roman';"><span lang="EN-US">-HAZ-</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">焊道</span><span style="font-family:'Times New Roman';"><span lang="EN-US">-HAZ-</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">母材。</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> 3&nbsp; &nbsp; </span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;"><span style="font-size:small;">結束語</span></span><span lang="EN-US"><br /> <span style="font-family:'Times New Roman';font-size:small;"> </span></span><span style="font-size:small;"><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">采用上述焊接工藝和焊接操作要領,在儀征化纖</span><span style="font-family:'Times New Roman';"><span lang="EN-US">45</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">萬噸</span><span style="font-family:'Times New Roman';"><span lang="EN-US">/</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">年</span><span style="font-family:'Times New Roman';"><span lang="EN-US">PTA</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">裝置施工過程中進行雙相不鏽鋼薄壁管現場施焊,取得了焊縫連續</span><span style="font-family:'Times New Roman';"><span lang="EN-US">5</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">個月</span><span style="font-family:'Times New Roman';"><span lang="EN-US">RT100%</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">合格,年度雙相不鏽鋼焊接接頭綜合合格率達到</span><span style="font-family:'Times New Roman';"><span lang="EN-US">99%</span></span><span style="font-family:宋體;mso-ascii-font-family:&quot;Times New Roman&quot;;mso-hansi-font-family:&quot;Times New Roman&quot;;">以上的施焊業績。</span></span> </p> <span style="font-family:宋體;font-size:small;"> </span>

西安雙相不鏽鋼管的焊接要求

在石油化工裝置中一種新型鋼材-雙相不鏽鋼的應用越來越多。因為雙相不鏽鋼的屈服強度是普通不鏽鋼的2倍,抗腐蝕性能(特彆是在腐蝕性介質中)明顯優於普通不鏽鋼,在石油化工裝置施工中多用在很重要的位置。因此,一般雙相不鏽鋼的焊縫要求100%RT檢驗,對其焊接接頭的綜合性能的要求也高於一般奧氏體不鏽鋼。所以,必須選派焊接經驗豐富的奧氏體不鏽鋼焊工,經培訓和考試合格後,才能持證上崗進行焊接作業。
1   
焊接性分析
雙相不鏽鋼焊接時,焊接熱影響區(HAZ 存在高溫區和低溫區,低溫區基本處於δ+γ(鐵素體+奧氏體)平衡組織,而高溫區幾乎為單相δ組織,因為焊縫根部和表麵N的擴散,導致靠近焊縫表麵的部位,由於N的損失,鐵素體增加,從而促進氮化物的產生,使焊接接頭性能惡化,焊接采用高線能量時,可以得到較多的γ相,鐵素體含量低會促進δ相產生,所以容易產生δ相和粗晶組織;線能量較低時,得不到足夠的γ相。如果焊接金屬中δ相過多,N很容易與形成化合物,而且析出二次γ變為針狀和羽毛狀,具有魏氏體組織特性,導致焊接接頭力學性能和耐腐蝕性下降。雙相鋼一般不會產生δ相,但如果焊接線能量較高,導致使焊接頭塑性大幅度下降。
2   
焊接工藝
2.1   
工藝參數及電特性(見表2
2.2   
焊接方法
雙相不鏽鋼薄壁管全部采用GTAW焊接,直流正極性。
2.3   
焊接設備
焊機采用高頻引弧焊機,直流正極性,鎢極直徑Φ2.5mm,鎢極端頭用磨光機磨出錐形,采用大噴嘴。
2.4   
氣體保護
焊接保護氣體采用混合氣體Ar97.5%+N2.5% 進行保護,保護氣采用成品混合氣,要求生產的成品混合比為Ar97.5%+N2.5%,由於混合氣體中ArN多,放置一段時間後將會產生分層,影響氣體保護效果,現場所采用搖勺或加氣體分配器進行配比,確保氣體保護質量。
2.5   
環境要求
雙相不鏽鋼焊接要求環境清潔。無鐵離子汙染,預置工作將在室內進行,地麵采用膠皮隔離、安裝必須做好環境保護。采用防風防塵設施,環境溫度70℃,相對溫度≤90%,所有與雙相鋼焊接坡口相接觸的,如:焊材、工具、手套等,都必須無鐵鏽汙染。坡口均采用坡口機加工,坡口角度為單邊30°±2.5°,鈍邊0~ 0.5mm,單麵坡口(見附圖),加工坡口不允許母材產生過燒變色;其兩側各50mm以內的內外表麵要進行嚴格清理,清理程序是磨光機打磨、丙酮(或無水乙醇)清洗,清洗後不能直接進行焊接作業,待坡口端麵晾乾後方可焊接作業;焊絲也用沾丙酮(或無水乙醇)的海綿擦拭乾淨。對鐵離子、水鏽、油、灰塵、油漆、記號筆印都必須清理乾淨,防止其影響化學成份和機械性能。另外,還要注意坡口形狀必須無凹凸和劃痕,這樣焊接時電弧在焊道的每一點上都能保證停留相同的時間,焊接線能量才能確保一致。
2.6   
焊接措施
儘量采用多層焊,因為後續焊道對前層焊道有熱處理作用,焊縫中的δ相進一步轉化為γ相,使焊接接頭的組織和性能顯著改善,而後一道焊縫處於非工作介質麵,因為對焊接接頭影響不大,保護氣采用Ar97.5%+N2.5%。因為焊接根部保護氣體中加氮氣增加焊縫金屬氮量,由於采用多層焊工藝,焊接材料中含N量與母材相當,而後一道焊縫處於非工作介質麵,因為對焊接接頭影響不大,采用合適的線能量焊接,使焊接接頭得到足夠的γ相,使N1 M有足夠的時間擴散。
2.7   
坡口的組對及點焊
坡口組對前應仔細檢查坡口管徑是否相同,錯邊應控製在0.5~1mm之間,並用磨光機打磨清理坡口及坡口正反麵兩側50mm以內的表麵,並用丙酮擦試乾淨,坡口打磨時不允許使母材產生過熱變色。點焊時,應采用與正式的焊接工藝相同的參數,點焊長度為7~8mm,高度為2~ 3mm,點焊點應為過橋型式,不應焊透,以防內部氧化,點焊電流不宜過大,點焊點位置應在組對管子的上部及兩側,點固三點,從第四點起焊,當焊到點焊時,將點固點打磨清理乾淨,焊縫組對間隙應控製在2~2.5mm,間隙不應過大,並留有0~0.5mm的鈍邊。
2.8   
雙相不鏽鋼的焊接操作
雙相不鏽鋼焊接時,應采用正反麵氣體保護焊,正麵背麵都應采用混合氣體Ar97.5%+N2.5% 進行保護,焊接前不得在焊件表麵引弧和試驗電流,焊接時應按指定的焊接作業指導書進行施焊。在焊接前,管子兩端用布或膠皮封好,並留有進氣孔和排氣孔,焊縫間隙用膠布貼好,並留有20~30mm的長度,使管子內部的空氣能夠排出,確保焊縫內部的氣體保護效果。焊接時,焊槍不宜擺動,手法要穩,嚴格控製線能量,儘量采用小焊絲,嚴格控製電流,弧長儘量壓低控製電壓,儘量用大噴嘴,提高氣體保護效果,降底O、H汙染;引、收弧避開點焊點,防止產生二次γδ相,引弧點必須在焊道內進行,不能在母材表麵引弧,防止F量超標;點焊點打磨後,封底焊焊接過程中通過觀察焊道顏色來確定焊接氣體保護效果,采用混合氣體施焊時焊道好為金黃色,稍差一些為黃銅色,儘量減少焊縫發藍,杜絕焊道發灰和發黑,並嚴格控製層間溫度,控製熔池在紅熱狀態下停留時間。一般來講,隻要保證在5~15s時間內熔池由紅轉至常規顏色,就能達到要求。打底焊的層間溫度≤100℃,可用遠紅外激光測溫儀測量。當層間溫度<100℃時,才能進行下一層焊接,焊接電流不能超過打底焊的電流,焊**層必須認真清理前一層焊道,除消除雜質外,連氧化色也需磨去,焊縫內部餘高應控製在0.5 ~1mm;焊縫收弧時應將弧坑填滿,多層焊的層間接頭應相互錯開,如果焊接作業時不慎出現夾鎢時,應停止焊接作業,用磨光機消除鎢點,鎢極端部重新磨尖,達到要求後方可重新進行焊接作業,要求與開始焊接作業相同。
2.9   
焊後清理和焊接檢驗
雙相不鏽鋼的焊後清理也很重要,氧化色必須**,因為氧化色下麵就是貧鉻層,若不去除將會導致耐蝕性能下降,去除氧化色可用專用不鏽鋼絲刷趁熱擦刷;也可用酸或酸洗膏清洗。去除焊接飛濺,打磨收起弧點,去除咬邊和粗毛刺。可用較細的砂輪片或拋光砂輪片研磨,杜絕粗糙打磨痕跡,否則易造成縫隙腐蝕;油汙、著色劑、色筆印、灰塵均有可能成為孔腐蝕和縫隙腐蝕的起始點,可用硝酸+氫氟酸清洗,然後清水衝洗乾淨;焊工應對焊道表麵進行清理,要求外觀良好,寬度以每邊蓋過坡口邊緣2mm為宜,角焊縫的焊腳高度符合設計規定外形平穩過渡,焊縫不允許咬邊、裂紋、未焊透、氣孔、夾雜存在。射線探傷方法按《壓力容器無損檢測》JB4730-g4執行,所有焊道必須進行硬度測定,測定母材-HAZ-焊道-HAZ-母材。
3   
結束語
采用上述焊接工藝和焊接操作要領,在儀征化纖45萬噸/PTA裝置施工過程中進行雙相不鏽鋼薄壁管現場施焊,取得了焊縫連續5個月RT100%合格,年度雙相不鏽鋼焊接接頭綜合合格率達到99%以上的施焊業績。

陝公網安備 61010402000326號

精品久久久无码中文字幕边打电话 | 一区二区av在线 | 日韩成人免费 | 亚洲综合日韩久久成人av | 青草青草久热国产精品 | 久久亚洲精精品中文字幕早川悠里 | 国产美女自拍视频 | 国产福利视频一区二区 | 欧美一区二区三区视频在线观看 | 亚洲国产良家在线观看 | 麻豆视频在线观看免费网站黄 | 黄网免费在线观看 | 日老女人视频 | 欧美精品乱码视频一二专区 | 中文字幕一区二区三区av | 小明www永久免费播放平台 | 国产91视频在线观看 | 亚洲视频手机在线 | 国产精品欧美久久久久无广告 | 在线观看黄a∨免费无毒网站 | 强被迫伦姧惨叫人妻系列 | 高清日韩欧美 | 99久久精品日本一区二区免费 | 苏小妍直播漏内裤 | 喷水视频在线观看 | 成人国产网站v片免费观看 欧美xo影院 | 欧美又粗又大又硬又长又爽视频 | 99热黄色| 熟妇女人妻丰满少妇中文字幕 | 日本韩国欧美中文字幕 | 又粗又黄又硬又爽的免费视频 | 亚洲国产欧美中文丝袜日韩 | 日韩在线不卡视频 | 亚洲成人第一区 | 亚洲sm另类一区二区三区 | 草草影院地址 | 97久人人做人人妻人人玩精品 | 色噜噜亚洲男人的天堂www | 国产高清女同学巨大乳在线观看 | 狠狠久久五月精品中文字幕 | 丰满少妇免费做爰大片人 | av不卡免费在线观看 | 嫩草影院黄色 | 国产亚洲美女精品久久久久 | 日韩一级色片 | 亚州性无码不卡免费视频 | av国产在线观看 | 国产私人尤物无码不卡 | 欧美肥老太牲交大战 | 在线黄av | 人人妻人人妻人人人人妻 | 性开放少妇xxx视频 91九色丨porny丨肉丝 | www黄色片| 国产成人综合亚洲亚洲国产第一页 | 91视频国产免费 | 哺乳一区二区久久久免费 | 亚洲成a人片在线视频 | 美脚の诱脚舐め脚责91 | 久久香蕉综合色一综合色88 | 新久小草在线 | 一级bbbbbbbbb毛片 | yy111111少妇嫩草影院 | 亚洲免费视频播放 | 日韩少妇乱码一区二区三区免费 | 熟女少妇人妻中文字幕 | 欧洲美女高清视频 | 99精品网| 黑人巨大精品欧美黑寡妇 | 国产又大又硬又粗无遮挡 | 在线观看的黄色网址 | 柠檬福利视频导航 | 性视频毛茸茸 | 特级丰满少妇一级aaaa爱毛片 | 黄色一二三区 | 九九综合 | 麻豆国产精品va在线观看不卡 | 92国产精品午夜福利无毒不卡 | 亚洲免费成人在线 | 国产高清精品综合在线网址 | 国产又粗又硬又大爽黄老大爷 | 国产欧美日韩亚洲一二三区 | 日本三级久久 | 插吧插吧网 | 7x7x7x人成影视 | 久久久麻豆精品一区二区 | 久久中文字幕人妻熟女凤间 | 性感美女毛片 | 亚洲最大综合网 | 国产片av国语在线观看导航 | 国产乱子伦农村叉叉叉 | 美国av毛片 | 欧美老女人性生活视频 | 国产一精品av一免费爽爽 | 黄色免费看视频 | 一本之道av不卡精品 | 日本三级韩国三级三级a级按摩 | 女人被弄到高潮的免费视频 | 亚洲精品国产欧美 | 91久久婷婷国产一区二区三区 | 久久亚洲精中文字幕冲田杏梨 | 亚洲成色最大综合在线 | 国产aⅴ爽av久久久久电影渣男 | 午夜av不卡 | 免费观看添你到高潮视频 | 三及片在线观看 | av无码免费无禁网站 | 综合一区无套内射中文字幕 | 激情综合色综合久久综合 | 少妇粉嫩小泬喷水视频在线观看 | a√视频在线 | 日韩乱论 | 国产日产精品一区二区三区四区的观看方式 | 亚洲精品久久久久avwww潮水 | 黄色日本视频 | 久久婷婷香蕉热狠狠综合 | 300部国产真实乱 | 久久与婷婷 | 伊人久久大香线蕉综合影视 | 丁香六月色 | 亚洲精品国产剧情久久9191 | 欧美日韩va | 久久99精品久久久久久清纯 | 日本成人精品 | 精品少妇人妻av久久久 | 日韩激情无码免费毛片 | 99国产精品99久久久久久 | 亚洲qvod激情经典在线观看 | 男女男精品网站 | 偷偷操不一样 | 天堂在/线资源中文在线bt | 免费视频色 | 免费在线观看你懂的 | 极品老师腿张开粉嫩小泬 | 久久久久久久亚洲国产精品87 | 欧美成人精品三级在线观看播放 | 国产露出视频 | 成在线人av免费无码高潮喷水 | 在线a人片免费观看 | 国产一区二区三区免费播放 | 蜜臀av88 | 思思久久99热只有频精品66 | 99久久爱re热6在播放 | 亚洲国产av玩弄放荡人妇 | 四川少妇被弄到高潮 | 亚洲综合色噜噜狠狠网站超清 | 中文字幕日韩在线视频 | 亚洲第一网站 | 国产一区二区三区四区三区 | 亚洲毛片一区二区三区 | 绿帽h啪肉np辣文 | 久久99精品国产麻豆 | 黄色视屏在线免费观看 | 国产aⅴ精品一区二区三区久久 | 麻豆一区二区三区蜜桃免费 | 亚洲精品久久久久久中文字幕 | 精品久久久久久777米琪桃花 | 97久久精品无码一区二区天美 | 麻豆剧场| 四虎国产精品永久在线下载 | 亚洲hdmi高清线 | 丰满护士巨好爽好大乳 | 国产一区二区视频在线播放 | 99久久精品久久久久久清纯 | 777色狠狠一区二区三区 | 国产免费视频精品视频 | 精品成人乱色一区二区 | 夜色综合 | 极品少妇一区二区三区 | 亚洲欧美国产双大乳头 | 噜噜噜久久久 | 亚洲男人的天堂成人www | 欧美日本日韩aⅴ在线视频 少妇高清一区二区免费看 免费看美女扒开屁股露出奶 | 日本免费在线观看视频 | 欧美aa大片欧美大片观看 | 欧洲人妻丰满av无码久久不卡 | 中文字幕人成无码人妻综合社区 | 成人国内精品久久久久影院vr | 91福利免费 | 免费的av在线 | 啪啪亚洲 | 富婆如狼似虎找黑人老外 | 成人小说亚洲一区二区三区 | 男女啪啪猛烈无遮挡猛进猛出 | 成人私密视频 | 色噜噜狠狠狠综合曰曰曰88av | 国产无遮挡又黄又爽在线观看 | 中文字幕一区二区三区乱码图片 | 亚洲a∨无码男人的天堂 | 黄色片aa | 呻吟揉丰满对白91乃欧美区 | 国产经典一区二区三区蜜芽 | 两性午夜免费视频 | 亚洲午夜久久久精品一区二区三区 | 国产极品美女高潮无套在线观看 | 亚欧中文字幕 | 天天爽天天摸天天碰 | 国产超碰在线 | 中文天堂最新版www 最新欧美精品一区二区三区 | 99视屏| 99久久久久久国产精品 | 麻豆国产av穿旗袍强迫女佣人 | 亚洲三级影视 | 国产区日韩区欧美区 | 浴室人妻的情欲hd三级国产 | 精品视频久久久久 | 国产又色又爽又刺激视频 | 久欠精品国国产99国产精2021 | 亚洲精品无码成人片 | 特级黄aaaaaaaaa毛片 | 国产男女猛烈无遮挡 | 国产一在线精品一区在线观看 | 无码人妻丰满熟妇区毛片18 | 久草在线视频免费资源观看 | 在线视频国产99 | 久久综合中文字幕 | 亚洲精品国产精品国产自2022 | 成人欧美在线观看 | 丰满岳乱妇在线观看视频国产 | 国产高清乱理伦片 | 久久精品爱 | 日韩黄色免费 | 欧美黑人疯狂性受xxxxx喷水 | 欧美猛交xxx| 伊人蕉影院久亚洲高清 | 久久久中文网 | xxxx野外性xxxx黑人 | 欧美性大战久久久 | 国产精品女同一区二区 | 久久婷婷五月综合色d啪 | 日本一道一区二区视频 | 一区二区三区四区在线 | 中国 | 一本大道伊人av久久综合 | 一级做a爰片久久毛片 | 亚洲大尺度无码无码专区 | a毛看片免费观看视频 | 国产麻豆天美果冻无码视频 | 穿情趣内衣c到高潮av片 | 亚洲 自拍 色综合图 12p | 精品熟女少妇av免费久久 | 麻豆视频在线观看免费 | 红桃视频91 | 免费激情 | 爱情岛论坛亚洲线路一 | 小鲜肉自慰网站 | 亚洲第一综合网站 | 国产乱子伦在线一区二区 | 高h破瓜受孕龙精 | 天天夜碰日日摸日日澡性色av | 欧美另类交人妖 | 亚洲午夜爱爱香蕉片 | 毛片在线播放视频 | 91麻豆精品国产91久久久点播时间 | 一本au道大尺码高清专区 | 精品视频一区二区三区在线观看 | 欧美1级片 | 全黄h全肉边做边吃奶视频 香蕉在线精品视频在线 | a级黄色网址 | 小荡货好紧好爽奶头大视频 | 最爽无遮挡行房视频 | 国产老师开裆丝袜喷水视频 | 亚洲色图av在线 | 韩国毛片基地 | 日本激情小视频 | 亚洲精品成人悠悠色影视 | 91avcom | www17c亚洲蜜桃 | 亚洲欧洲成人a∨在线观看 在线亚洲日产一区二区 | 5566先锋影音夜色资源站在线观看 | 欧洲亚洲1卡二卡三卡2021 | 久久亚洲国产成人影院 | 好紧好爽再进去一点在线视频 | 色站综合| 97国产精品自拍 | 久久这里只有精品首页 | 毛片网站在线免费观看 | 99精产国品一二三产品香蕉 | 亚洲经典一区二区 | a在线视频播放观看免费观看 | 亚洲第一男人天堂 | 国产日韩中文字幕 | 国内丰满少妇猛烈精品播 | 久久久久久久9 | 宅男午夜成年影视在线观看 | 国产精品成人va在线观看 | 2018国产精华国产精品 | 日本日皮视频 | 亚洲伊人一区 | 催眠调教后宫乱淫校园 | 99mav| 男人爽女人下面动态图 | 亚洲午夜视频 | 欧美成人免费观看 | 亚洲九色| 丰满人妻被黑人中出849 | 老司机精品福利视频 | 亚洲咪咪 | 综合久久婷婷 | 99久久免费精品国产男女性高好 | 91欧美日韩综合 | 国精产品999永久天美 | 久久亚洲熟女cc98cm | 日韩视频福利 | 久久国产精品精品国产色婷婷 | 韩日av一区二区 | 超碰在线94| 永久av在线 | 亚洲香蕉 | 日本色区 | 国产熟妇搡bbbb搡bb七区 | 夜夜嗨av一区二区三区 | 午夜在线欧美蜜桃 | 国产精品视频一区二区在线观看 | 76少妇精品导航 | 最近免费韩国日本hd中文字幕 | 上原亚衣av一区二区三区 | 成人无码精品一区二区三区亚洲区 | 午夜无码伦费影视在线观看果冻 | 国产亚洲欧美人成在线 | 国产丝袜一区二区三区免费视频 | 三a大片 | 色偷偷成人| 91精品在线免费观看 | 两个人看的www免费视频中文 | 妩媚尤物娇喘无力呻吟在线视频 | 色欲色香天天天综合vvv | 国产精品人成视频免费软件 | 国产9色在线 | 日韩 | 久久综合给合久久狠狠狠97色69 | 欧美成人精品在线观看 | av天堂久久天堂色综合 | 精品成人免费视频 | 亚洲视频小说 | www.91色.com| 天天干干 | 五月婷婷丁香 | 亚洲人成77777在线播放网站 | 午夜激情视频网站 | 久久久亚洲色 | 久久综合九色综合网站 | 国产suv精品一区二av18款 |